**Author:** ![YankeeDoodleDinghy](https://avatars.discourse-cdn.com/v4/letter/y/da6949/32.png) [@YankeeDoodleDinghy](https://forum.clcboats.com/u/YankeeDoodleDinghy)\
**Post date:** [September 17, 2026, 3:13pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/1 "2026-09-17T15:13:13Z")

</div>

Hi, I’m a first time builder, sander, and painter. I’m working on a Tenderly Dinghy. I have a question about sanding my hull before painting.

(My current paint plan: marine primer (unless there are reasons this would be bad), anti-fouling paint below the waterline, and then light-colored marine topcoat above the waterline. I want her to look good not sloppy, but I don’t need it to look professional-level.)

Question: If I’m painting the hull, how important is it to have the same level of sanding perfection that is needed for good brightwork? Especially if I’m planning primer? Of course I do plan on re-epoxying any areas sanded-through to weave or raw wood, and re-sanding those areas, since doing this makes the boat more durable. The question: is it necessary to eradicate those small glossy pits, that seem to pop up everywhere?

These tiny pits seem more cosmetic, and I’d imagine that the primer would smooth those out well enough. Plus, trying to sand smooth those tiny pits is increasing my sand-throughs to fiberglass or raw wood… creating additional work that I’d like to avoid. Thanks.

---

<div class="post-metadata">

**Author:** ![Jon\_Ferguson](https://avatars.discourse-cdn.com/v4/letter/j/d9b06d/32.png) [@Jon\_Ferguson](https://forum.clcboats.com/u/Jon_Ferguson)\
**Post date:** [September 17, 2026, 3:59pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/2 "2026-09-17T15:59:49Z")

</div>

Primer helped me suss out areas that needed attention that were sort of hidden before the primer. I’ve never fooled with anti-fouling paint, I would follow the directions on the can as closely as possible. I’ve heard some anti-fouling paints don’t like primer.

---

<div class="post-metadata">

**Author:** ![Laszlo\_Morocz](https://avatars.discourse-cdn.com/v4/letter/l/c68b51/32.png) [@Laszlo\_Morocz](https://forum.clcboats.com/u/Laszlo_Morocz)\
**Post date:** [September 18, 2026, 12:28am UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/3 "2026-09-18T00:28:05Z")

</div>

Primer is to fill in pinholes and to make the paint bond better to the epoxy. Epoxy-compatible paints don’t need a primer.

For the best paint job you want to use fairing compound. You can make your own from epoxy and phenolic microballoons or buy a pre-mixed compound. I prefer making my own because I can control the proportions as required by different parts of the boat. For example, a slightly thinner compound for the bottom of the boat so it’ll cure harder, a thicker compound for the sides so they won’t sag, etc. In any case, once the fairing compound cures, sand it with a manual fairing board for the best results. You’ll probably sand off most of the compound and leave only what is needed to fill in the valleys to match the hills. If you sand to #220 grit you’ll also be taking care of the pinholes and can skip the primer.

Finally, anti-fouling bottom paint. You only need it if you will be keeping the boat in the water for weeks at a time. For a Tenderly I’d recommend non-ablative paint because the boat is slow compared to motor boats and the paint (and growth) won’t be pulled off by the motion of the water. Since you’re going to have to scrub/pressure wash anyway, might as well use the more environmentally friendly paint.

Alternatively, pull the boat out once a week and scrub it and don’t worry about anti-fouling paint. Coat the bottom with McLube Hullkote and you expand that to 4 weeks (at least in Maryland waters).

Laszlo

---

<div class="post-metadata">

**Author:** ![Steve\_Sawtelle](https://avatars.discourse-cdn.com/v4/letter/s/edb3f5/32.png) [@Steve\_Sawtelle](https://forum.clcboats.com/u/Steve_Sawtelle)\
**Post date:** [September 18, 2026, 9:15am UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/4 "2026-09-18T09:15:40Z")

</div>

When you say ‘small glassy pits’ are you referring to small depressions that the sander didn’t hit? If so, they should be sanded. A scotch bright pad will get down in those areas and scuff up the surface enough to get a good mechanical bond with the next layer, be it fairing, primer, or paint.

I also agree about the fairing. It sands easily and is not a hard step to do. Makes a big difference in the finish. Don’t rely on your paint to hide any thing.

---

<div class="post-metadata">

**Author:** ![YankeeDoodleDinghy](https://avatars.discourse-cdn.com/v4/letter/y/da6949/32.png) [@YankeeDoodleDinghy](https://forum.clcboats.com/u/YankeeDoodleDinghy)\
**Post date:** [September 20, 2026, 4:05pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/5 "2026-09-20T16:05:37Z")

</div>

Thank you very much. Below are two picture examples of what I mean by small glossy pits. When I’ve sanded some other areas with similar defects, I’ve accidentally burnt through the epoxy to fiberglass or wood, obviously not ideal.

First of all, will the fairing compound (or primer or paint) hide these defects, and I should just leave them alone for now? Or, will these small defects show through fairing / primer, etc, and I should deal with them now, buy either sanding them more with a sander, or as you mention with scotch bright pad… or, as an alternative, I could also apply more epoxy on top of them, and then sand that? Many options to think about, thanks.

Also, when reading about fairing compound, I’d thought of it as being good for larger gaps and hills. Is it as beneficial if the hull, in general, has a good shape, and it’s just these smaller imperfections that I’m hiding? Or would primer or just paint alone be good enough? Thanks again!

 ![20260920_115207](https://canada1.discourse-cdn.com/flex007/uploads/clc/original/2X/8/8a61177bc9632fe5fe4bd54585e638c412dd7d03.jpeg)

 ![20260920_115057](https://canada1.discourse-cdn.com/flex007/uploads/clc/original/2X/7/7901ec0dbee0d5d9a199a3ef6d0b3c094a35478f.jpeg)

---

<div class="post-metadata">

**Author:** ![Laszlo\_Morocz](https://avatars.discourse-cdn.com/v4/letter/l/c68b51/32.png) [@Laszlo\_Morocz](https://forum.clcboats.com/u/Laszlo_Morocz)\
**Post date:** [September 20, 2026, 4:42pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/6 "2026-09-20T16:42:36Z")

</div>

Those defects will definitely show through paint. They are too big for primer (primer is for pinhead-sized holes). Epoxy/microballoon mix will definitely fill them in. You could fill them in with epoxy, but that’s heavier, more expensive (since epoxy costs more than microballoons) and much harder to sand (since cured epoxy is harder than phenolic).

For painted glass-covered plywood boats the main benefits of fairing compound are:

- Filling the weave
- Smoothing out and unevenness in glass application
- Smoothing out places where one sheet of glass overlaps onto another
- Filling in defects like the ones you posted.

For your next painted glass-covered boat, stop with the epoxy after the glass is on and before you fill the weave. Go directly to filling the weave with a single thick coat of epoxy/microballoon mix and sand it with a fairing board. You’ll be combing all the finish steps from filling the weave to fairing to paint prep into one. That’s how I did this boat.

 ![wr18](https://canada1.discourse-cdn.com/flex007/uploads/clc/original/2X/3/30ff6cf87e45f767b58e92a20fae9f3daba24639.png)

---

<div class="post-metadata">

**Author:** ![YankeeDoodleDinghy](https://avatars.discourse-cdn.com/v4/letter/y/da6949/32.png) [@YankeeDoodleDinghy](https://forum.clcboats.com/u/YankeeDoodleDinghy)\
**Post date:** [September 20, 2026, 6:22pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/7 "2026-09-20T18:22:26Z")

</div>

That’s a gorgeous boat. Looks like it’s moving fast, even when it’s sitting still.

For fairing compound, how thick a microballoon / epoxy mixture would you use to cover areas with these tiny holes scattered across it, like my hull? Also, for smoothing fiberglass overlaps, how thick a mixture would you recommend?

How do you recommend people handle the increased porosity of the microballoon fairing compound, when it comes to preparing for the next step of paint or varnish?

Am I right that the microballoons in the fairing compound don’t change the way light travels through the epoxy mixture, and don’t make the epoxy mixture more translucent or opaque… in other words, am I right that builders can still finish with varnish on top of the fairing compound, and the wood will show through the same as without the fairing compound?

Thanks much

---

<div class="post-metadata">

**Author:** ![Jon\_Ferguson](https://avatars.discourse-cdn.com/v4/letter/j/d9b06d/32.png) [@Jon\_Ferguson](https://forum.clcboats.com/u/Jon_Ferguson)\
**Post date:** [September 20, 2026, 6:37pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/8 "2026-09-20T18:37:15Z")

</div>

Micro ballon’s make epoxy look tan/white they definitely show up through varnish.

 ![IMG_3774](https://canada1.discourse-cdn.com/flex007/uploads/clc/original/2X/7/75ac04286b8f3b57487bc11deb1323c8aa88bd7f.jpeg)

---

<div class="post-metadata">

**Author:** ![Laszlo\_Morocz](https://avatars.discourse-cdn.com/v4/letter/l/c68b51/32.png) [@Laszlo\_Morocz](https://forum.clcboats.com/u/Laszlo_Morocz)\
**Post date:** [September 20, 2026, 8:18pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/9 "2026-09-20T20:18:27Z")

</div>

What Jon said. Fairing compounds are just for painted finishes. They are **not** for a varnished finish. In your first post you asked “_If I’m painting the boat…_” That’s why I’ve been going on about fairing compounds. If you’re varnishing, you need to do all the filling, fairing and finish with epoxy, right up until applying the varnish.

But if you’re painting and using epoxy/microballoon mix, I like to mix mine to the consistency of room temperature canned cake frosting. I apply it with a squeegee, just as if I were frosting a cake. If it’s difficult to apply (rolls up under the squeegee, for example) I just add a very little epoxy to loosen it up.

I don’t worry about increased porosity. I know some people do because they think that sanding opens the microballoons, but those things are microscopic in size. You need magnifying equipment to see them and the hollow spaces inside are even smaller. The resulting holes are so small that paint can easily fill them.

Laszlo

---

<div class="post-metadata">

**Author:** ![Robert\_Whitehurst](https://avatars.discourse-cdn.com/v4/letter/r/85e7bf/32.png) [@Robert\_Whitehurst](https://forum.clcboats.com/u/Robert_Whitehurst)\
**Post date:** [September 21, 2026, 1:15am UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/10 "2026-09-21T01:15:53Z")

</div>

I used the purple micro balloon fairing mixed with the Mas epoxy on my paddleboard. I f’d up enough glass work on the bottom of the board that I gave up on the standard epoxy and sand and filled the goofs with the fairing compound, sanded and painted with Brightsides.

I will make a proposal for using flattening agent in the paint. I did that on my skerry and it hides many smaller paint errors. Obviously you won’t get the high gloss look but use the boat a bit and you may appreciate the semigloss ability to hide small scuffs and errors.

---

<div class="post-metadata">

**Author:** ![YankeeDoodleDinghy](https://avatars.discourse-cdn.com/v4/letter/y/da6949/32.png) [@YankeeDoodleDinghy](https://forum.clcboats.com/u/YankeeDoodleDinghy)\
**Post date:** [October 6, 2026, 6:56pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/11 "2026-10-06T18:56:50Z")

</div>

Thank you. Three quick follow up questions.

When you apply the cake-frosting fairing compound, on the hull, how thick a layer are you putting with the squeegee.

I think I read that the mixture need to be thicker when applied to vertical surfaces, like the hull near the stem, how much thicker, about?

I’m in a very warm environment, does the fairing compound tend to cure faster or slower than other epoxy mixtures, such as the woodflour, for example? Unfortunately I’m always racing against the clock to apply my epoxy before it’s becoming hot. Thanks!

---

<div class="post-metadata">

**Author:** ![Matt\_Adam](https://avatars.discourse-cdn.com/v4/letter/m/4af34b/32.png) [@Matt\_Adam](https://forum.clcboats.com/u/Matt_Adam)\
**Post date:** [October 10, 2026, 5:13pm UTC](https://forum.clcboats.com/t/sanding-epoxy-before-paint-perfection-needed/72399/12 "2026-10-10T17:13:25Z")

</div>

Nice work on the Tenderly for a first build, and taking the time to fair those pits now will really pay off once the paint goes on.